Titanium Stress Corrosion Cracking: The Three-Thing Trap

Titanium stress corrosion cracking (SCC) needs three things at the same time: tensile stress, a specific chemical medium, and a susceptible alloy in a susceptible condition. Remove any one and the crack stops. That is why a Ti-6Al-4V part can survive a stronger acid in a beaker and still crack in a mild-looking methanol line years later — the load was residual from welding, and the medium was anhydrous. The counter-intuitive evidence is sharper than the warning. A NATO materials record on rocket-oxidiser tanks reports that N2O4 cracking at about 105°F and stress near yield was controlled by adding roughly 0.6% NO or 1% water, and that glass-bead shot peening worked while changing the alloy did not. Water makes the film repairable; removing it makes the metal defenceless. This guide names the three media that matter — methanol with halides, red fuming nitric acid and N2O4, and hot salt — separates SCC from ordinary corrosion and fatigue, and ends with a twelve-line RFQ.

How to read this guide. We are a stockholder and light fabricator in Baoji, not a fracture laboratory and not a designer of oxidiser tanks or aircraft structure. Every figure below is tied to its medium, stress or temperature and to the named source. SCC is probabilistic and depends on geometry, surface condition and stress state, so no single safe stress or life number is printed here. Where the evidence is a laboratory result rather than a field rule — the hot-salt compressor studies, for example — we say so. Use this to frame the right question for a corrosion engineer or design authority, not to clear a part for service.

At a Glance: The Ten Facts That Decide an SCC Question

Item Figure or finding Why it matters Status
Three conditions Tensile stress + specific medium + susceptible alloy/condition Remove one, SCC stops Framework, not a warranty
Dangerous stress Often RESIDUAL from welding or cold work Can exceed the applied design load Why a low-stressed part still cracks
Methanol + halides Gr2/Gr4 sensitive (Sedriks, ASM 13A) Anhydrous is the trigger Methanol becomes an active SCC agent
The water paradox Adding ~1% H2O makes methanol/N2O4 innocuous TiO2 film can then self-repair NATO AGARD-CP-53
N2O4 Cracked at ~105 F near yield stress Green (NO-rich) safer than red 0.6% NO inhibitor specified
Red fuming nitric acid Risk when <1.5% water or >6% NO2 Ti prohibited for such lines in defence use Rolled Alloys / Donachie
Hot salt SCC Ti alloys susceptible 200-500 C Ti-6Al-4V prone above 250 C Joseph/Rolls-Royce; IIT Bombay
Grade split CP Gr2/Gr7 near-immune to chloride SCC Gr5 (alpha-beta) susceptible Why CP lines seawater, not Gr5
Mitigation that worked Glass-bead shot peening (N2O4 tanks) Changing alloy did not Surface compressive stress
What this does not give No single safe stress or KISCC value Specimen and geometry dependent Ask for data in your medium

How to use this table: the first two rows are the frame — three conditions, and residual stress hiding in plain sight. For the pure-medium side without load, see our failure casebook; this guide is about what happens when a medium and a stress act together.

1. The Short Answer: Three Things, One Sudden Crack

Stress corrosion cracking is not ordinary corrosion accelerated by load. It is a separate mechanism in which a specific chemical medium and a tensile stress together allow a crack to grow through metal that is otherwise passive and apparently sound. The surface often looks intact right up to failure, which is why SCC is treated as one of the more dangerous modes in process and aerospace equipment.

The practical frame is a three-part test: is there tensile stress (including residual stress from welding or forming), is the medium one of the specific SCC agents, and is the alloy in a susceptible condition? If any answer is no, ordinary SCC is off the table. Our quote comparison guide shows how a process choice becomes a price; here the process choice is what decides whether a crack can grow at all.

2. The “Titanium Never Cracks” Myth

Titanium’s reputation comes from a TiO2 film that makes it close to immune in seawater, wet chlorine and many oxidising acids. That reputation is deserved for corrosion. It does not transfer to SCC, because the three-condition test is different from a corrosion-rate table. A part can sit in a mild-looking solvent for years and then crack because the solvent was anhydrous and the weld carried near-yield residual stress.

Condition Role in SCC Mitigation lever Where it hides
1. Tensile stress Applied load OR residual stress Compressive stress suppresses cracking Welding, cold work and fit-up matter
2. Specific medium Not just "corrosive" - a named chemistry Methanol+halide, RFNA, N2O4, hot chloride Seawater alone is usually kind to Ti
3. Susceptible alloy + condition Alpha-beta Gr5 more than CP; high strength/oxygen worse Widmanstatten & high O more sensitive Grade AND temper must be named
All three present Cracks initiate and grow below yield Little visual warning before failure The reason SCC is feared
One removed SCC does not initiate Change medium, stress state or alloy The whole mitigation logic

The third row is the one buyers miss. Grade equivalence tells you how a Chinese grade maps to ASTM or EN; it does not tell you the SCC behaviour of the temper. The condition — annealed, solution treated and aged, cold worked, oxygen level — belongs on the enquiry as surely as the grade name.

If a medium or stress state might match this guide, the enquiry needs those lines up front. Copy these fields so a supplier can answer with service conditions rather than a grade name.

What to send us for an exact titanium quote

Copy these nine lines into your enquiry. A complete spec means a firm price on the first reply, not a second email asking for the grade.

Spec item Example from a real order
Grade Grade 2 (UNS R50400), commercially pure titanium
Standard ASTM B265 / ASME SB-265, current revision
Form & Size Plate, 6 mm × 1000 mm × 2000 mm, hot-rolled and annealed
Quantity 500 kg (12 sheets), one-off batch
Service medium & temperature Seawater, 30 °C, continuous immersion
MTC type EN 10204 3.1, heat-specific, with melt chemistry and tensile values
Inspection Third-party witness (SGS / BV) before dispatch; PMI on request
Target delivery Ex-works within 5 working days; FOB Shanghai on request
Drawing DXF of cut-to-size blanks, tolerance ±1.0 mm, edges deburred

Ready? Copy the nine lines above into the Requirement Details box on our Request a Quotation page and we will come back with a firm price and a dispatch date within 24 hours.

3. The Water Paradox: Removing Water Removes Protection

The sharpest result in the public record is also the least intuitive. In rocket-oxidiser service, adding a small amount of water made titanium safer, not less safe. The reason is film chemistry: the TiO2 layer self-repairs only when water is present. Take the water away and a cracked film cannot reform, so the exposed metal keeps reacting.

Condition What changed Effect on SCC Source / reading
N2O4, "green" (NO-rich) About 0.6% NO specified as inhibitor Cracking greatly reduced NATO AGARD-CP-53
N2O4 + ~1% H2O Water raises effective NO in equilibrium Non-corroding N2O4 achievable Same record
N2O4, "red" (high purity) Low NO, near-anhydrous SCC incidence increased sharply Mechanism: oxide cannot self-repair
Methanol, anhydrous No water; halide impurity present Active stress-corrodant for Ti Titanium methoxide is soluble
Methanol + small H2O Water added deliberately Rendered innocuous Allows TiO2 film repair
Reading Removing water removes protection Not an alloy problem - a film-chemistry problem Control the medium first

This is why a supplier asking “how much water is in the methanol?” is asking a better question than one quoting a corrosion resistance rank. It is also a mitigation that costs almost nothing: change or inhibit the medium before changing the metal. See our service temperature guide for the separate question of how long titanium keeps its strength when hot.

4. Medium One: Methanol and the Halide Trigger

Pure methanol is not the problem. Methanol with halide impurities — chloride, bromide or iodide — is. Sedriks and the ASM Handbook, as summarised in the corrosion literature, record commercially pure Grades 2 and 4 as highly sensitive to SCC in methanol-halide mixtures. Fine chemical and pharmaceutical plants that use methanol as a solvent with chloride contamination are exactly the setting where the risk appears.

The NATO record explains the mechanism: in the absence of water the reaction product between titanium and methanol is titanium methoxide, which is soluble and gives no protection. Cracking started at the surface without needing a pre-existing notch, and required enough stress to deform the metal so fresh surface was exposed. The same record says adding a little water rendered the methanol innocuous. Our heat exchanger page and coil selection guide are the product forms where a solvent line question usually begins.

5. Medium Two: Red Fuming Nitric Acid and N2O4

Red fuming nitric acid and nitrogen tetroxide are oxidisers, not ordinary process acids. Rolled Alloys’ Ti-6Al-4V data sheet notes SCC susceptibility in methyl alcohol, red fuming HNO3 and N2O4, and says the nitric-acid problem is limited to environments with less than 1.5% water or more than 6% NO2. Donachie’s technical guide is blunter: titanium alloys are not used for pipelines handling fuming nitric acid in defence and explosive service.

The NATO record on N2O4 tanks gives the field detail. Cracking appeared at a moderately elevated 105°F with wall stress approaching the yield strength of the tank material. Higher-purity “red” N2O4 increased SCC markedly compared with “green” N2O4, whose higher NO content protected it; the oxidiser used subsequently carried a specified ~0.6% NO. Adding ~1% water was another route to non-corroding N2O4. Surface-initiated cracking needed no notch or precrack, and the recommended practical controls were environmental plus glass-bead shot peening. This is oxidiser-service evidence; hand any such duty to a qualified design authority.

6. Medium Three: Hot Salt on Turbine and Process Parts

Hot-salt SCC is the one most relevant to aerospace and gas-turbine buyers. Joseph, Lindley, Dye and Saunders at Imperial College with Rolls-Royce state that titanium alloys are susceptible when exposed to halides in the 200 to 500°C range, and that the first report was Ti-6Al-4V creep-tested at 370°C. Their Ti-6246 work found cracks initiating beneath salt particles in the presence of oxidation, with oxygen, chlorine and sodium enrichment at the site.

Study / condition Finding Detail Source
150-400 C slow-strain test Ti-6Al-4V prone above 250 C Crack count and length rise from 300 C IIT Bombay / GTRE, AMPP 2013
370 C creep test HSSCC first reported in Ti-6Al-4V Classic early observation Cited by Joseph et al., Imperial College
200-500 C window Ti alloys susceptible with halides Aero/marine/industrial gas turbines Joseph / Rolls-Royce, Ti-6246 study
350 & 450 C, 520 MPa bend stress Below alloy yield; salt droplet applied Initiation beneath salt particles Same Ti-6246 two-point-bend rig
288-427 C band Sensitive range quoted for Ti flanges High-Al/high-O, coarse Widmanstatten worse CXMET producer note; verify for your alloy
Lab vs engine Mostly seen in lab samples, rarely service Flow may remove products; compressor pressure favours oxidation Joseph et al.; not a service exemption

The same paper notes an important nuance: hot-salt SCC is mostly seen in laboratory samples rather than aircraft components, possibly because airflow removes corrosion products or compressor pressure favours oxidation over the moisture reaction that charges hydrogen. That is an explanation for a field observation, not a licence to ignore it. Our aerospace fastener rod page and Grade 5 bar page are where high-strength bar questions start.

If a specific medium and a stressed part are already on the drawing, send both to our request a quotation page. A named engineer will confirm in writing which grades and conditions we can supply from stock and where a corrosion engineer or design authority must decide — within 24 hours.

7. Where the Stress Comes From: Residuals Beat the Drawing

In SCC failures the applied stress shown on the drawing is often not the stress that started the crack. Welding, cold forming, machining and fit-up leave tensile residual stress in the surface, sometimes approaching the alloy’s yield strength. The N2O4 case is the clean example: the tanks cracked at about 105°F under wall stress near yield, and a surface compression treatment helped while changing the alloy did not.

Stress source Effect Consequence Control
Welding residuals Lock-in tensile stress near yield Often the real cause in tanks and pipework Stress-relieve and peen where allowed
Cold work / forming Surface tensile layer Bends and cold-expanded holes at risk Anneal after severe cold work
Machining / grinding Surface tensile stress + smeared layer Same surface factor as fatigue Control tooling and final finish
Fit-up and preload Assembly bolts, press fits Slower but persistent Specify torque and sequence
Applied operating load Pressure, rotation, thermal cycles What the drawing accounts for Usually smaller than residuals at the crack
Compressive surface Shot peening, glass bead Worked in the N2O4 tank case AGARD record; specify coverage and intensity

This puts SCC on the same surface-dependence footing as fatigue. Our fatigue and surface integrity guide covers how the last machining or grinding step can dominate fatigue life; here the same surface state decides whether a crack can initiate at all. The heat treatment guide explains the annealed and STA conditions that sit behind the strength numbers.

8. The KISCC Idea: Why “Below Yield” Is Not Safe

Engineers new to SCC often assume that keeping stress below yield strength is enough. It is not. Fracture mechanics describes a threshold stress intensity, written KISCC, below which a crack of a given size will not grow in a given environment. Above it, a crack can grow slowly at stress levels well below yield. Reported thresholds vary widely with alloy, microstructure, specimen type and medium: one study of a Ti-24Al-11Nb intermetallic in methanol reported KISCC/KIC ratios around 0.53 to 0.69, but that is a titanium aluminide, not a standard Grade 2 or Grade 5 value.

The honest conclusion is that there is no single safe stress number to print in an article. The threshold depends on the flaw size your inspection can actually detect, the part geometry, and the exact medium. Ask your supplier for test data on the product form and condition you are buying, and have the design authority set the allowable stress. Our bar receiving UT page shows how flaw detection is specified on incoming material.

9. Grade Choice: Why CP Lines the Seawater Line

The grade split in SCC is the opposite of the strength split. Commercially pure Grades 1 and 2, and palladium-bearing Grade 7, are near-immune to chloride SCC at ambient temperature, which is a major reason they line seawater and brine equipment rather than the stronger Grade 5. Ti-6Al-4V, an alpha-beta alloy, is susceptible in methanol, red fuming nitric acid, N2O4 and hot chloride, and higher-strength conditions can be more sensitive.

Grade family SCC behaviour Where it is susceptible Typical use
CP Gr1/Gr2 (alpha) Near-immune to ambient chloride SCC Sensitive in methanol+halides, hot salt at temperature Default for seawater/brine
Gr7 (Ti-0.15Pd) CP-level chloride immunity + crevice resistance Not a cure for methanol or RFNA Reducing-acid and crevice duty
Gr12 (Ti-Mo-Ni) Better hot-brine crevice resistance Still not an SCC-free alloy Hot brine / geothermal
Gr5 / Ti-6Al-4V (alpha-beta) Susceptible in methanol, RFNA, N2O4, hot chloride Strength does not remove SCC - can worsen condition effects Aero, fasteners, high-strength parts
Gr23 (Ti-6Al-4V ELI) Lower interstitial, higher toughness Conservative stress levels still required Fracture-critical use
Near-alpha (Ti-6242, Ti-6246, IMI834) Designed for hot strength, not SCC immunity HSSCC studied in 200-500 C range Compressor / turbine components

Where Grade 5 is genuinely needed for strength in a chloride environment, the common engineering response is the ELI grade plus conservative stress levels, with the decision owned by the designer. Grade 7 solves crevice corrosion and reducing-acid duty, not methanol or fuming nitric acid. Our Grade 2 vs Grade 7 seawater page and Grade 12 plate page set out the corrosion-led comparison; add the SCC question on top.

10. The Hydrogen Link: SCC, Fatigue and Embrittlement Overlap

The hot-salt studies make a connection that matters for how you investigate a failure. Joseph and colleagues detected hydrides precipitated on cooling and concluded that hydrogen produced by the salt-titanium reaction was responsible for cracking. The IIT Bombay work describes transgranular fracture through alpha grains up to 350°C and mixed intergranular and transgranular fracture higher up. So a mechanism called stress corrosion can end in a hydrogen-embrittlement fracture, and the crack can then advance by a fatigue-like process.

That overlap is why surface condition, residual stress and medium chemistry recur across our guides. This article handles the coupled medium-and-stress case; the melt practice guide explains how ingot condition and inclusions affect fatigue-critical stock, and the traceability guide covers how heat identity is preserved. None of them replaces a fracture investigation on the actual part.

11. Mitigation That Worked, and Mitigation That Did Not

The most useful hierarchy in SCC is also the cheapest: change the medium first, then the stress state, then the alloy. The NATO record is unusually clear on this. For red N2O4, modifications to the alloy and its condition had not been effective, while glass-bead shot peening the inside of the tanks, which introduces surface compression, worked reasonably well. For methanol, switching to another pressurising liquid removed the problem entirely.

That ordering is worth copying in a plant. Inhibiting or drying a medium, stress-relieving a weld, or specifying controlled peening can all be cheaper and more certain than changing to a different titanium grade. Whatever is chosen must be documented: peening needs coverage and intensity, stress relief needs a temperature and time that do not undo the grade’s properties, and medium control needs a measured water or inhibitor content. The welding wire page and EN 10204 3.1 certificate page are where consumable and heat documentation start.

12. When This Guide Stops

SCC is safety-relevant, so the boundaries matter more than in a general material article.

Situation Why this guide is not enough What to do instead
Treating “titanium does not rust” as “it cannot crack” SCC leaves the surface looking intact Name the medium and stress state on the RFQ
Buying high-strength Gr5 for a warm chloride line Alpha-beta is the SCC-sensitive family Consider CP or Gr7 and confirm with the designer
Ignoring welding and cold-work residuals Residual stress can approach yield Specify stress relief, peening or anneal
Using anhydrous methanol for hydrotest Halide traces turn it into an SCC agent Use water, or inhibit and document it
Assuming a passive film repairs in every liquid No water, no self-repair in methanol/N2O4 Control the medium chemistry first
Quoting a KISCC number without geometry Threshold depends on specimen, flaw and condition Ask for data on your actual part
Clearing a safety-critical part from an article Aircraft and oxidiser duties need design authority Route to a qualified engineer

The last row is the governing one. Aircraft structure, rotating turbine parts, rocket oxidiser tanks and pressure boundaries are designed and signed off by qualified engineers using the applicable code. An article can help you ask whether SCC is in scope; it cannot clear a part for service.

13. A Twelve-Line SCC RFQ

Send these with the drawing. Lines 1, 2, 4 and 10 carry most of the risk, because they describe the medium chemistry and the stress state that a grade name alone never captures.

# Field Example entry
1 Exact medium + impurities Methanol + 200 ppm Cl, or RFNA NO2 %
2 Water content wt% H2O - often the deciding variable
3 Temperature range Ambient / 250-500 C hot-salt band
4 Stress state Applied, residual, weld, cold-work, peened
5 Grade + condition Gr2 annealed / Gr5 STA / Gr23 ELI
6 Product and geometry Tank, tube, fitting, bolted flange, notch radius
7 Surface finish and treatment Pickled, machined, shot-peened, glass-beaded
8 Flaw / inspection basis UT or PT method, acceptance standard, detectability
9 Test basis offered Slow strain rate, constant load, ASTM G36/G38 if relevant
10 Design code / authority Which code sets allowable stress and who signs off
11 Mitigation accepted Inhibit medium, stress relieve, peen, change grade
12 Consequence class Safety-critical / pressure / tractable leak - who reviews

Line 10 deserves emphasis. If a code sets the allowable stress, name it, and name who signs off a change. A supplier who asks for the medium, the water content and the welding condition is engaging with the SCC question; one who only quotes a grade is answering a different one.

14. Choose CP / Choose Gr5 / Choose a Different Route

Choose commercially pure Grade 2 or Grade 7 when ambient seawater, brine or oxidising chemistry drives the choice and SCC resistance matters more than strength. Start with Grade 2 plate, condenser tube or Grade 12 plate for the relevant form. Our weight calculator guide helps quantify the section once a grade is chosen.

Choose Grade 5 or Grade 23 ELI when strength is genuinely required, accepting that the alpha-beta family is the SCC-sensitive one. Name the temper, the surface condition and the inspection basis; keep the stress decision with the design authority. See Grade 5 bar and Ti-6Al-4V bar stock.

Choose a medium or process change when the chemistry is the trigger: dry or inhibit methanol, specify N2O4 inhibitor, or remove the halide source. This is often the highest-value lever and the one most often missed.

Choose a different material when the medium is red fuming nitric acid or another environment where titanium is explicitly not used. A supplier who will say so is more useful than one who will quote any grade.

15. Why Source This From Us

We are a stockholder plus light fabricator in Baoji, the centre of China’s Titanium Valley. We will not sell titanium into an SCC-sensitive duty on the strength of a corrosion table alone:

  • We ask about the medium. Roughly 800 t of titanium, nickel and zirconium stock across plate, tube, bar, wire, fittings, flanges and fasteners, and we ask what exactly is in the fluid and how much water it contains.
  • We name the condition. Grade, temper, surface finish and inspection basis travel together on our quotations, because condition is part of the SCC question.
  • We say when another party must decide. Aerospace, oxidiser and pressure-boundary duties belong to the design authority, not to a material supplier.
  • Certificates match the metal. EN 10204 3.1 MTC per heat, heat numbers hard-stamped, and inspection reports aligned with the same heat.
  • Technical answers in 24 hours. Send the medium and stress state and we will tell you which grades and conditions we can supply from stock and where a specialist must sign off.

Start with B265 plate, titanium bar, welding wire or nickel alloy stock; each page lists the forms and certification that matter for that product.

Get a firm titanium quote within 24 hours

Same-day dispatch from ~800 t of Baoji stock  ·  cut-to-size and waterjet blanks  ·  free drawing review by our engineering team  ·  EN 10204 3.1 MTC with every lot.

Request my quote →

No obligation. A named engineer replies, not an auto-responder.

EN 10204 3.1 MTC on every lot  ·  ISO 9001 quality system  ·  ASTM / ASME / GB standard literacy  ·  Third-party inspection (SGS / BV) on request  ·  Mill heat & lot traceability  ·  Export packing & full documentation

16. FAQ: Titanium Stress Corrosion Cracking

What three things does titanium SCC need?

Tensile stress, a specific chemical medium, and a susceptible alloy in a susceptible condition. Remove any one and stress corrosion cracking does not initiate. The stress is often residual from welding or cold work rather than the applied design load. The medium must be named, not just called corrosive: anhydrous methanol with halides, red fuming nitric acid, N2O4 and hot halides are the classic cases. Ti-6Al-4V in the alpha-beta family is more susceptible than commercially pure grades, and higher strength or oxygen content can make the condition worse.

Why does adding water make methanol and N2O4 safer for titanium?

Because titanium relies on a thin TiO2 film that needs water to repair itself. In anhydrous methanol with halide impurities, the reaction product is titanium methoxide, which is soluble and not protective; the film cracks and cannot regrow. A NATO materials record notes that adding a small amount of water renders methanol innocuous, and that N2O4 with about 0.6% NO inhibitor or roughly 1% water becomes non-corroding. This is a medium-chemistry fix, not an alloy fix.

Is Ti-6Al-4V suitable for seawater if it is SCC susceptible?

Commercially pure Grade 2 and Grade 7, not Grade 5, are the default for seawater and brine lines. The alpha-beta Grade 5 is susceptible to chloride SCC at temperature and in specific media such as methanol and red fuming nitric acid. Where Grade 5 is required for strength in chloride service, designers commonly specify the ELI grade and keep stress intensity below the SCC threshold, with the decision belonging to the design authority. Do not treat the grades as interchangeable on strength alone.

At what temperature does hot salt stress corrosion start?

Published work puts titanium alloy susceptibility to hot salt SCC broadly in the 200 to 500 C range. A slow-strain-rate study at IIT Bombay found Ti-6Al-4V prone above 250 C, with crack count and length rising from 300 C. An Imperial College and Rolls-Royce study of Ti-6246 tested at 350 and 450 C under a 520 MPa surface stress below the alloy yield, and found cracks initiating beneath salt particles. These are laboratory conditions; a service decision needs your alloy, stress and environment reviewed by a qualified engineer.

Does shot peening actually prevent SCC?

It can help, but it is not a universal fix. The NATO record on N2O4 tankage reports that glass-bead shot peening, which puts the surface into compression, was reasonably effective at reducing SCC susceptibility, while modifications to the alloy and its condition were not. That makes sense because SCC here starts at the surface. The result is specific to that oxidiser and that stress state; if peening is used, specify coverage, intensity and how it will be verified, and confirm it with your design authority.

How is SCC different from fatigue and hydrogen embrittlement?

Fatigue is crack growth under cyclic load; SCC needs a static tensile stress plus a specific medium; hydrogen embrittlement is damage from hydrogen entering the metal. They can overlap: the hot-salt studies attribute cracking to hydrogen produced when halides hydrolyse at temperature, and SCC can then propagate by a fatigue-like mechanism. This is why surface condition, residual stress and medium chemistry appear in all of them. Our fatigue guide covers the cyclic-load side and the traceability guide covers how heat and grade identity are proven.

What should I put on an RFQ for SCC-sensitive service?

Give the exact medium and its impurities, water content, temperature range, stress state including welding and cold work, the grade and temper, product geometry and notch radius, surface finish and any peening, the inspection method and acceptance basis, the design code and who signs off, and the consequence class of a leak. Ask the supplier what SCC or slow-strain-rate test basis they can offer in your medium. A twelve-line checklist turns a grade question into an answerable service question.

Summary: Ask About the Medium and the Stress, Not Just the Grade

Titanium SCC needs three things at once — tensile stress, a specific medium, and a susceptible alloy and condition — and removing any one stops it. Residual stress from welding or cold work often matters more than the applied load. Anhydrous methanol with halides, red fuming nitric acid (<1.5% water or >6% NO2), N2O4 and hot halides in the 200-500 C band are the named risks; Ti-6Al-4V becomes prone to hot-salt SCC above 250 C. The most counter-intuitive fix is in the medium: about 0.6% NO or 1% water made N2O4 non-corroding in the NATO record, and a little water rendered methanol innocuous because the TiO2 film can then repair. CP grades resist ambient chloride SCC while alpha-beta Grade 5 does not; shot peening worked in the oxidiser-tank case where changing the alloy did not. No single safe stress is published here — send the twelve-line SCC checklist through our request a quotation page and a named engineer will confirm supply from stock within 24 hours.

Need a Quote? Message Us Directly

Get live stock status, price and lead time — usually the same business day. No form required, just tap to chat.