There is no single maximum service temperature for titanium. Ask ten suppliers and you will hear 300°C, 400°C, 540°C and 649°C — and each number can be defended, because each answers a different question. The oxidation limit (where air starts attacking the metal) for commercially pure titanium is about 649°C, with visible colour change from 371°C; the strength-retention limit is roughly 315°C for Grade 2 and 400°C for Grade 5; the code allowable stress for an ASME SB-338 Grade 2 tube is capped at 600°F (316°C) and falls as temperature rises; and 540°C belongs to Ti-6242 near-alpha alloy, not to pure titanium. Treating these as one number is how a vessel gets specified too hot or a good alloy gets scrapped too early. This guide separates the four lines, gives the source and boundary for each, and ends with what to write on an RFQ so the temperature question is answered in writing.
How to read the numbers. We are a stockholder and light fabricator in Baoji, not a standards body and not a design authority. Temperatures below are published producer and code figures reproduced with the source named in the field table; where a code value is quoted it is for orientation only. A real allowable stress or service limit depends on the product form, section, code edition, load case and inspection regime. For any pressure boundary or safety-related part, the governing code edition and a qualified engineer decide. Our job here is to stop you comparing unlike numbers.
| Question | Number | What it really means | Source / status |
|---|---|---|---|
| Oxidation begins (colour) | ~371°C / 700°F | Light straw colour in air | TIMET, first-hand |
| Heavy oxide layer | ~426°C / 800°F | Oxygen diffuses into lattice | TIMET, first-hand |
| Loses oxidation resistance | >649°C / 1200°F | Becomes brittle, not a service limit | TIMET, first-hand |
| Rapid scale | ~927°C / 1700°F | Fast scaling | TIMET, first-hand |
| Gr2 strength retention | ~315°C (600°F) | Creep/strength, not oxidation | indicative; sources differ |
| Gr5 strength retention | ~400°C (750°F) | Ti-6Al-4V, AMS-based | indicative; verify |
| ASME SB-338 Gr2 tube | 600°F / 316°C cap | Code allowable stress limit | ASME Sec II Part D |
| ASME allowable stress fall | 14.3 → 6.5 ksi | Gr2 seamless tube, 100°F → 600°F | ASME Sec II Part D |
| The “540°C” number | Ti-6242 alloy | Near-alpha service ceiling, NOT pure Ti | common mix-up |
How to use this table: find the question you are actually asking, then read that line only. A supplier quoting 649°C to justify a hot-air vessel and a supplier quoting 316°C to size a code tube are not contradicting each other — they are answering different questions. For why grade names alone mislead, see our grade equivalence guide.
When someone asks for “the maximum service temperature of titanium”, the honest answer is a question back: do you mean the point where air attacks it, the point where it loses too much strength, the point where it creeps under load, or the point your pressure code allows? Those four boundaries sit at very different temperatures, and all four are legitimate.
The table separates them. Line 1 is chemistry — oxygen attacking the surface. Line 2 is short-term mechanical strength. Line 3 is time-dependent deformation. Line 4 is what a code will sign off. A part is limited by the lowest line that applies to its service, not by the highest number on the internet. This is the single most useful thing to carry into a temperature conversation.
| Line | Question it answers | Typical number | Source class | When it governs |
|---|---|---|---|---|
| 1. Oxidation / air attack | Where the metal is consumed or embrittled by oxygen | >649°C loss of resistance | TIMET producer data | Any hot air / oxygen service |
| 2. Strength retention | Where short-term yield/tensile falls too far | Gr2 ~315°C, Gr5 ~400°C | indicative, multi-source | Load-bearing parts |
| 3. Creep | Where slow strain under load becomes life-limiting | Gr5 useful ~150°C+ under sustained load | code allowables decline with T | Sustained stress, long life |
| 4. Code allowable stress | What the pressure code legally permits | SB338 Gr2 tube 600°F cap | ASME BPVC Sec II Part D | Pressure vessels, boilers |
Keep the four columns distinct in your specification. The failure casebook shows what happens when the medium is right but the temperature or surface condition is wrong; this guide is the temperature half of the same problem.
Titanium’s colour under heat is a real physical signal, but it is a process indicator, not a design allowance. TIMET’s published data gives the boundaries: excellent resistance in air and oxygen up to about 700°F (371°C), where a light straw colour appears; a heavy oxide layer may form at 800°F (426°C) as oxygen diffuses through the lattice; above 1200°F (649°C) the metal lacks oxidation resistance and becomes brittle; and scale forms rapidly at 1700°F (927°C).
| Temperature | What happens in air | Mechanism | Engineering meaning |
| Up to ~371°C / 700°F | Excellent resistance in air and oxygen; light straw colour at 700°F | Protective film intact | Reference boundary only |
| ~426°C / 800°F | Heavy oxide layer may form; oxygen diffuses through the lattice | Film thickens, colour blue | Avoid if surface or fatigue matters |
| >426°C | Oxidation accelerates with time; scale builds and spalls | Protect, or remove after | Vacuum / inert for critical parts |
| >649°C / 1200°F | Lacks oxidation resistance, becomes brittle from oxygen absorption | Embrittlement, irreversible | Hard limit for air exposure |
| ~927°C / 1700°F | Scale forms rapidly | Severe attack | Outside any service envelope |
The trap is reading 371°C as “the limit” because that is where colour appears. Colour change is not failure; it is the surface film thickening. The genuine hard boundary for air exposure is 649°C. Our annealed versus STA guide covers the same oxide layer when it forms during manufacturing; here the concern is heat during service.
A number that circulates in forums and some datasheets is 540°C as “the maximum temperature of titanium”. That figure comes from Ti-6242 (Ti-6Al-2Sn-4Zr-2Mo), a near-alpha alloy with silicon additions used for compressor discs and blades, where it is a reasonable approximate service ceiling. It is not a property of commercially pure titanium, and it is not an oxidation boundary.
The confusion matters in both directions. Specifying Grade 2 plate for 540°C air service because “titanium handles 540” is unsafe; the metal loses oxidation resistance above 649°C and loses useful strength far below that. Conversely, rejecting a Ti-6242 component at 500°C because “titanium is limited to 400” throws away a qualified high-temperature alloy. The grade has to be named before the temperature question means anything. Our Grade 5 bar page and bar stock overview make the grade distinction explicit.
If a temperature is already written into your specification, send it with the medium and the grade. Copy these fields into your enquiry so every supplier answers the same question.
|
What to send us for an exact titanium quote Copy these nine lines into your enquiry. A complete spec means a firm price on the first reply, not a second email asking for the grade. |
||||||||||||||||||||
|
||||||||||||||||||||
|
Ready? Copy the nine lines above into the Requirement Details box on our Request a Quotation page and we will come back with a firm price and a dispatch date within 24 hours. |
Strength retention asks a simpler question than oxidation: at temperature, is the metal still strong enough for the load? Published figures put commercially pure Grade 2 at roughly 300 to 315°C and Grade 5 at about 400°C for sustained service. These are indicative numbers, not code allowables, and they move with product form and design basis.
| Grade / alloy | Approx. useful ceiling | Typical use | Status of the number |
|---|---|---|---|
| Grade 2 (CP) | ~300–315°C | Low-stress chemical equipment, tube, plate | Sources differ 300 vs 315; verify |
| Grade 5 (Ti-6Al-4V) | ~400°C (750°F) | Aerospace structure, compressor blades | indicative, AMS-based |
| Grade 9 (Ti-3Al-2.5V) | ~350°C | Aircraft ducting, tubing | indicative |
| Ti-6242 (6-2-4-2) | ~540°C | Compressor discs, blades, casings | near-alpha + Si |
| IMI 834 | ~600°C | Highest-temperature rotating Ti parts | near-alpha, specialty |
Note the spread in the Grade 2 row: 300°C and 315°C both appear in public sources. We will not pick one for you. Write the governing code and edition into the enquiry and let the design authority confirm the value. What this table does establish is the ordering: pure titanium sits below Grade 5, and both sit far below the specialised near-alpha alloys.
Creep is time-dependent deformation under sustained stress, and it is the reason a part can be chemically untouched and still fail. Titanium’s creep resistance is limited relative to nickel superalloys; Grade 5 becomes life-limiting under long-term load well before its oxidation limit, which is why near-alpha alloys with silicon additions were developed for the 500 to 600°C range.
The practical consequence: a short tensile test at 400°C does not qualify a part for thousands of hours at 400°C under stress. If your component carries a sustained load at temperature, ask for creep or allowable-stress data at your specific stress and design life, not a generic maximum. Our fatigue guide covers the related case where cyclic load and surface condition, not heat alone, set the life.
For a pressure boundary, none of the metallurgical limits above decide the design. The governing pressure code does. ASME Section II Part D publishes allowable stresses for ASTM/ASME SB-338 Grade 2 titanium tube, with a stated maximum applicable metal temperature of 600°F (316°C). The allowable stress falls steadily with temperature.
| Metal temperature | Seamless, ksi | Welded, ksi | Note |
|---|---|---|---|
| −20 to 100°F | 14.3 | 12.1 | Baseline |
| 200°F | 12.4 | 10.6 | — |
| 300°F | 10.3 | 8.8 | — |
| 400°F | 8.8 | 7.5 | — |
| 500°F | 7.6 | 6.5 | — |
| 600°F (316°C) | 6.5 | 5.5 | Maximum applicable temperature |
These values are reproduced from a tube supplier’s transcription of ASME Section II Part D and are shown for orientation only — verify against the current code edition before use. The shape of the table is the lesson: allowable stress at 600°F is less than half the low-temperature value. Two quotes can differ simply because one was priced at ambient allowable stress and the other at the design temperature. The condenser tube page and welded versus seamless guide show the product forms this applies to.
Contradictions between temperature numbers are usually not errors; they are answers to different questions expressed without the question. A vessel designer quoting 316°C is protecting a code calculation. A metallurgist quoting 649°C is describing oxidation. An alloy specialist quoting 540°C is talking about Ti-6242. None of them is wrong in context.
Do three things. First, name the grade. Second, state which line governs: oxidation, strength, creep or code. Third, where published values conflict, such as the 300 versus 315°C Grade 2 ceiling, write the conflict into the enquiry and ask the supplier to confirm against the named code edition. That is the same discipline used for the standard conflicts in our grade equivalence guide and the cost differences in our quote comparison guide.
Oxidation is not the only high-temperature oxygen risk. In oxygen-enriched atmospheres titanium can ignite and burn. Published TIMET data cites a reported finding that ignition could not be induced even at very high pressure when oxygen content was below 35%, but also warns that once a reaction starts it propagates at much lower oxygen levels than those needed to start it, and that steam as a diluent allowed the reaction to proceed at still lower oxygen levels.
The highest-risk surfaces are fresh ones — a fracture face, a heavy scratch, a freshly machined edge — where the protective film is absent and oxidation is rapid and exothermic. If heat is given off faster than it can be conducted away, the surface can begin to melt and the reaction becomes self-sustaining. This is why oxygen service is a design discipline of its own and why the colour chart on this page must not be read as a fire-safety boundary. Ask for oxygen-service cleaning and design practice where it applies; see also our heat exchanger page for equipment context.
Temperature changes which media are dangerous, not just how fast they attack. Three cases are worth knowing because they surprise buyers who assume titanium is inert.
| Medium | Temperature threshold | Failure mechanism | Control |
| Oxygen / air | ~371°C colour, >649°C brittle | Ignition risk in high O2; <35% O2 reported non-ignitable even at high pressure | Protect fresh surfaces; avoid high-O2 at heat |
| Hydrogen | >77°C (170°F) pick-up becomes significant | Hydriding if pH <3 or ≥12, abraded surface, or cathodic potential; H solubility ~100–150 ppm Gr2 | Keep oxide film intact; control pH and potential |
| Nitrogen | Gold film >538°C (1000°F); diffusion >816°C (1500°F) | Nitride diffusion can embrittle | Avoid pure N2 at high heat |
| Ammonia | >150°C (302°F) decomposes to H + N | Absorbed H causes embrittlement; high corrosion in NH3-steam at 220°C | Do not assume Ti is inert to hot ammonia |
Hydrogen is the most common of the three. Below about 77°C pick-up is so slow it has no practical significance, but above it — with pH below 3 or above 12, an abraded surface, or a cathodic potential — hydriding becomes a real risk. The hydrogen solubility limit for Grade 2 is around 100 to 150 ppm, beyond which hydrides precipitate. The failure casebook covers the medium-side failures; add temperature to that map before you sign a service condition.
If you would rather not map four limits against your own service, send the grade, temperature, medium and code through our request a quotation page. A named engineer will tell you in writing which limit governs and what we can supply from stock — within 24 hours.
If the duty genuinely requires 500 to 600°C under load, the answer is not a different temperature rating for Grade 2. It is a different alloy. Near-alpha alloys such as Ti-6242 and IMI 834 were developed specifically to push the creep and oxidation ceiling upward, combining a predominantly alpha microstructure with silicon additions for creep resistance.
These are specialty, aerospace-qualified products with controlled processing and certification, not general stock items. If a supplier offers ordinary Grade 5 plate for a 550°C sustained-load application, that is a specification problem, not a bargain. Be candid with your supplier about whether the part is a rotating aerospace component or a static chemical vessel; the qualification burden and the price are entirely different. Our nickel and titanium alloy stock page and Baoji exporter page show the product families we hold for less extreme duties.
Two oxygen-related phenomena are routinely conflated. Alpha case is a hard, oxygen-enriched brittle layer formed during high-temperature processing — forging, heat treatment or hot working in air — and it must be removed by machining or pickling. In-service oxidation is the scale and oxygen diffusion that build up while the part is operating hot.
They share a mechanism but not a context, and the fix is different. Alpha case is a manufacturing defect to prevent or remove before the part ships; our heat treatment guide and plate ordering guide address that side. In-service oxidation is a design and inspection question: what temperature, for how long, with what surface protection and removal interval. Confusing the two leads buyers to reject a correctly heat-treated part for a service condition, or to accept heat tint on a weld that should have been removed.
This is a map of which limits exist, not a substitute for the value that governs your part. There are cases where the numbers here should not be used at all.
| Situation | Why this guide is not enough | What to do instead |
|---|---|---|
| Pressure boundary / boiler | Code allowable stress governs, not oxidation limit | Use current ASME edition + qualified engineer |
| Rotating aerospace part | Creep + fatigue + certification, not a chart temperature | Use qualified alloy and approved data |
| Sources disagree on Gr2 ceiling | 300°C vs 315°C vs higher published | State the conflict; verify against your code |
| Coating or cladding present | Limit may be the coating, not the titanium | Ask supplier for the coating limit |
| Zirconium or nickel service | Different temperature and media limits entirely | Use the right material guide |
| Fire / oxygen-enriched line | Ignition risk not captured by a temperature number | Design to oxygen-service practice |
The second row deserves emphasis: for rotating or certified aerospace parts, creep, fatigue, fracture mechanics and a qualified material specification interact in ways no single temperature table captures. If the part fails, people will ask for the approved data, not a webpage. Our mill certificate page explains the document trail we provide on stock material; it is evidence of chemistry and heat, not a design approval.
Send these fields together and the temperature question gets a factual answer instead of a generic number. Line 12 is the one most often omitted and the one that saves the most time.
| # | Field | Example entry |
|---|---|---|
| 1 | Alloy grade and product form | Gr2 plate / Gr5 bar / Gr2 SB338 tube |
| 2 | Media and whether air/oxygen present | Air, inert, chloride brine, high-O2 |
| 3 | Continuous and peak metal temperature | 280°C continuous / 320°C upset |
| 4 | Internal pressure and load case | Pressure boundary vs structural |
| 5 | Governing code and edition | ASME VIII-1, SB338, current edition |
| 6 | Sustained-load / creep requirement | Design life and stress level |
| 7 | Thermal cycling frequency | Start/stop count per year |
| 8 | Welded or seamless, and heat tint control | Back-gas purged, tint removed |
| 9 | Surface finish and inspection | Pickled/passivated, PT, RT |
| 10 | Certificate and traceability | EN 10204 3.1 MTC, heat number |
| 11 | Destination and standard | ASTM / ASME / GB / EN named |
| 12 | Which limit is actually governing | Oxidation vs strength vs code — state it |
Line 3 should give both continuous and upset temperature; a short excursion is not the same duty as a continuous one. Line 6 separates a hot vessel from a hot load-bearing part. With those twelve fields, a supplier can say which of the four lines governs your case and whether their stock is suitable. That is the conversation worth having before price.
Choose commercially pure Grade 2 or Grade 12 if the duty is corrosion-driven, the metal temperature stays below roughly 300°C, and there is no sustained high stress. Most chemical vessels and condensers live here. Start with Grade 2 plate or Grade 12 plate.
Choose Grade 5 (Ti-6Al-4V) if strength-to-weight matters and the temperature sits below about 400°C, with creep checked for any sustained load. Aerospace structure and high-strength components live here.
Choose a near-alpha alloy such as Ti-6242 or IMI 834 if the duty genuinely needs 500 to 600°C under load and you can carry the qualification and cost. That is specialised territory, not a stock substitution.
We are a stockholder plus light fabricator in Baoji, the centre of China’s Titanium Valley. We will not quote a single temperature that ignores which line governs:
Start with plate, tube, bar or equipment; each page lists the forms, sizes and standards that matter for that product.
|
Get a firm titanium quote within 24 hours Same-day dispatch from ~800 t of Baoji stock · cut-to-size and waterjet blanks · free drawing review by our engineering team · EN 10204 3.1 MTC with every lot. |
Request my quote →
No obligation. A named engineer replies, not an auto-responder. |
|
EN 10204 3.1 MTC on every lot · ISO 9001 quality system · ASTM / ASME / GB standard literacy · Third-party inspection (SGS / BV) on request · Mill heat & lot traceability · Export packing & full documentation |
There is no single number. For commercially pure titanium the oxidation limit in air is about 649 degrees Celsius, where it loses oxidation resistance and becomes brittle. But strength retention limits Grade 2 to roughly 315 degrees Celsius and Grade 5 to about 400 degrees Celsius, and the ASME code caps a Grade 2 SB-338 tube at 600 degrees Fahrenheit, which is 316 degrees Celsius. The governing number depends on whether you are worried about oxidation, strength, creep or code compliance.
In air, published TIMET data says titanium above 1200 degrees Fahrenheit, about 649 degrees Celsius, lacks oxidation resistance and will become brittle from oxygen absorption. A separate mechanism is hydrogen embrittlement, which becomes significant above 170 degrees Fahrenheit, about 77 degrees Celsius, when the oxide film is damaged and the environment is very acidic or very alkaline. These are different mechanisms with different temperature thresholds.
No. That figure belongs to Ti-6242, a near-alpha titanium alloy used for compressor discs and blades, as an approximate service ceiling. It is not the oxidation point of pure titanium, which is about 649 degrees Celsius, and it is not a limit that applies to Grade 2 or Grade 5 plate and tube. Applying 540 degrees Celsius to commercially pure titanium is a common and potentially unsafe mix-up.
For a pressure application to ASME SB-338, the published maximum applicable metal temperature is 600 degrees Fahrenheit, about 316 degrees Celsius, and the allowable stress falls from roughly 14.3 ksi at low temperature to about 6.5 ksi at 600 degrees Fahrenheit for seamless tube. That is a code figure for a pressure boundary, not the temperature at which the metal would oxidise. Confirm against the current code edition for your design.
Yes, creep becomes life-limiting under sustained load as temperature rises. That is why the useful temperature of Grade 5 under long-term stress is lower than its short-term strength would suggest, and why near-alpha alloys with silicon additions were developed for 500 to 600 degrees Celsius service. Creep is a separate limit from oxidation: a part can be perfectly oxidation-resistant and still fail by creep.
With caution. Above about 150 degrees Celsius ammonia decomposes into hydrogen and nitrogen, and the hydrogen can be absorbed and embrittle titanium. In pure nitrogen, a gold-coloured nitride film forms above about 538 degrees Celsius and diffusion can cause embrittlement above about 816 degrees Celsius. Do not assume titanium is inert just because it performs well in ambient ammonia or nitrogen service.
State the alloy and product form, the continuous and peak metal temperature, the media including whether oxygen is present, pressure and load case, the governing code and edition, and whether the limit you care about is oxidation, strength, creep or code compliance. Add weld and inspection requirements and the MTC type. With those fields a supplier can answer in writing instead of quoting a single generic number.
Titanium has no single maximum service temperature; it has four limits, and the lowest applicable one governs. Oxidation in air becomes a hard boundary above about 649°C, with colour change from 371°C; strength retention puts Grade 2 near 315°C and Grade 5 near 400°C; creep limits sustained-load parts lower still; and the ASME code caps an SB-338 Grade 2 tube at 600°F (316°C) with falling allowable stress. The widely quoted 540°C belongs to Ti-6242 near-alpha alloy, not pure titanium. Send the twelve-line checklist through our request a quotation page; a named engineer will tell you which limit governs and what we hold in stock within 24 hours.
Titanium Weight Calculator — Quick Reference
All values use density 4.51 g/cm³ (commercially pure and most Ti alloys). For Gr5 / Ti-6Al-4V (4.43 g/cm³) multiply by 0.982. Figures are theoretical; actual weight varies with tolerance and surface condition.
1. Plate & Sheet — weight per square metre
Formula: kg/m² = thickness(mm) × 4.51
| Thickness (mm) | 0.5 | 0.8 | 1.0 | 1.5 | 2.0 | 3.0 | 4.0 | 5.0 |
|---|---|---|---|---|---|---|---|---|
| kg/m² | 2.26 | 3.61 | 4.51 | 6.77 | 9.02 | 13.53 | 18.04 | 22.55 |
| Thickness (mm) | 6.0 | 8.0 | 10.0 | 12.0 | 15.0 | 20.0 | 25.0 | 30.0 |
| kg/m² | 27.06 | 36.08 | 45.10 | 54.12 | 67.65 | 90.20 | 112.75 | 135.30 |
Per full sheet: kg = T(mm) × width(mm) × length(mm) × 4.51 ÷ 1,000,000.
2. Round Bar — weight per metre
Formula: kg/m = diameter²(mm) × 0.00354
| Diameter (mm) | 6 | 8 | 10 | 12 | 15 | 20 | 25 | 30 |
|---|---|---|---|---|---|---|---|---|
| kg/m | 0.127 | 0.226 | 0.354 | 0.509 | 0.796 | 1.415 | 2.211 | 3.183 |
| Diameter (mm) | 40 | 50 | 60 | 80 | 100 | 150 | 200 | — |
| kg/m | 5.659 | 8.843 | 12.73 | 22.64 | 35.37 | 79.58 | 141.48 | — |
3. Tube / Pipe — weight per metre
Formula: kg/m = (OD − wall)(mm) × wall(mm) × 0.01414
| Size (OD × wall, mm) | 25.4×1.2 | 25.4×1.65 | 25.4×2.0 | 38×1.5 | 38×2.0 |
|---|---|---|---|---|---|
| kg/m | 0.411 | 0.554 | 0.662 | 0.775 | 1.018 |
| Size (OD × wall, mm) | 57×2.0 | 57×3.0 | 60.3×2.0 | 89×3.0 | 114×3.0 |
| kg/m | 1.555 | 2.291 | 1.647 |
Contact Person: Wang Xiaoning
Tel: +86-917-355-7966
Email: [email protected]
WhatsApp: +86 188 2967 9311
Company: Shaanxi Qianyi Tuoda Technology Co., Ltd
Address: Floor 4, Building 4, No. 188 Gaoxin Avenue, High-tech Zone, Baoji City, Shaanxi Province, China