Welcome to Shaanxi Qianyi Tuoda Technology Co., Ltd
EnglishРусский中文
Titanium Metal News

Titanium Traceability: Heat Numbers, PMI and the Invisible Mix-Up Risk

A titanium mix-up is invisible. Grade 2 and Grade 5 can share the same mill finish, the same weight to within 2% (4.51 versus 4.43 g/cm³), and no magnetic response — so sight, a magnet and a file cannot tell them apart. What separates them is a chain of evidence: a heat number from the melt, a mill certificate that names it, a marking that survives cutting, and a measurement on the actual metal. The certificate proves what the paperwork says; PMI (positive material identification) proves what the metal says; the heat number is the only thing that ties the two together. Break the chain at any point — most often at cut-to-size — and a fully certified bar becomes a pile of unidentifiable pieces. This guide shows where the chain breaks, what an XRF gun can and cannot establish, how the requirements differ by industry, and what to write on an RFQ so traceability is a contractual answer rather than a promise.

How to read this guide. We are a stockholder and light fabricator in Baoji, not a certification body, not a testing laboratory and not a design authority. Standards and instrument capabilities below are reproduced with the source named in the field table; acceptance limits are not invented here. The mix-up story is a titanium producer’s own published account, not an independent incident investigation. PMI is a verification tool, not a substitute for the mill certificate, and a handheld reading is not an arbitration result. For any safety-critical or code-certified part, the governing specification and an authorised inspector decide.

At a Glance: The Nine Facts That Decide Traceability

Item Value / scope What it means Status
Density gap, Gr2 vs Gr5 4.51 vs 4.43 g/cm³ (<2%) Weight and touch cannot identify the grade multi-source, indicative
Heat number One melt, one identifier The spine linking metal to certificate mill practice
MTR / mill certificate Document compliance Says what the mill recorded at the melt EN 10204 3.1 / 3.2
PMI by XRF Physical chemistry check Says what the surface actually contains API RP 578 programme
XRF reads well V, Mo, Ni, Pd, Fe Separates Gr5 / Gr7 / Gr9 / Gr12 instrument-dependent
XRF cannot read C, N, O, H Cannot separate Gr2 from Gr23 ELI needs lab methods
XRF does not prove Heat treatment / strength PMI verifies chemistry, not performance scope limit
Common break point After cutting to size Marked plate becomes unmarked pieces marking transfer needed
Weld consumables Separate verification Correct plate + wrong filler still fails API RP 578 scope

How to use this table: start with the two rows that matter most — a certificate proves paperwork, PMI proves chemistry, and neither works alone. For how the grade names themselves map across standards, see our grade equivalence guide.

1. The Short Answer: Traceability Is a Chain, Not a Certificate

A mill certificate is a document. It is excellent evidence of what the mill recorded, and useless on its own if the piece in your hand cannot be tied to it. Traceability is the chain that makes that tie: melt, heat number, product marking, certificate, any cutting operation, receiving inspection, and the records that survive all of them.

The chain is only as strong as its weakest link. A perfect certificate attached to an unmarked offcut is not traceability; a clean XRF reading on an unmarked bar is not traceability either. Both halves have to meet at the same heat number. That is the whole subject of this guide, and it is why a supplier who answers “yes, full traceability” without naming the marking method has not actually answered you.

2. The Invisible Mix-Up: A Producer’s Own Account

A titanium producer in Baoji published an account of a mix-up found during bar production. Five bars of Grade 2, about 23 kg in total, of the same 23 mm by 3,050 mm size as a Grade 5 order, had entered the wrong batch. The company describes stopping production, recalling finished goods already in transit, asking customers to hold stock, and tracing back to the originating furnace heat. This is the producer’s own published story, not an independent investigation, but the mechanism it describes is the industry’s standard fear.

Nobody in that story identified the wrong grade by looking at it. That is the point. Grade 2 and Grade 5 can arrive with the same surface, the same diameter and nearly the same weight. The mix-up only became visible once someone checked identity against a heat and an instrument. Our failure casebook covers what a wrong material does in service; this guide is about catching it before it gets there.

3. Why Sight, Magnets and Files Do Not Work

Three informal tests circulate in workshops. All three fail for titanium in ways that give false confidence rather than no answer.

Grade pair Appearance Density gap Real separator Correct method
Grade 2 vs Grade 5 Nearly identical <2% (4.51 / 4.43) Al ~6%, V ~4% in Gr5 XRF or OES on clean metal
Grade 1 vs Grade 4 Nearly identical Negligible Oxygen and iron limits Lab chemistry, not handheld XRF
Grade 5 vs Grade 23 (ELI) Nearly identical Negligible Interstitial O, N, H limits Lab inert-gas fusion / combustion
Grade 2 vs Grade 7 Nearly identical Small Palladium addition in Gr7 XRF or lab spectroscopy for Pd
Grade 9 vs Grade 5 Nearly identical Small Al and V levels (3/2.5 vs 6/4) OES or calibrated XRF

A magnet tells you almost nothing: neither commercially pure titanium nor Ti-6Al-4V is strongly magnetic in normal stock condition. A file or scratch test is subjective, and hard surface treatments such as nitriding or PVD can make even a soft grade “skate”. Weight is no better: our weight chart shows why a section that differs by less than two percent in density cannot be sorted by handling. Colour is a surface treatment, not an identity test. Only a chemistry measurement answers the question.

4. The Spine of the Chain: What a Heat Number Actually Is

A heat is one melt in a furnace. The mill analyses it and records its chemistry and mechanical results against a unique identifier: the heat number. Every later document refers back to that number. If the number is missing, the certificate becomes a generic sheet of numbers that could belong to any melt of that grade.

Stage What happens What must be preserved Evidence
1. Melt Heat is poured and analysed Chemistry is recorded against one heat number Mill heat log
2. Mill product Plate, bar or tube is made Heat number is stamped, etched or tagged on the product Physical mark
3. Certificate MTR / CMTR is issued Heat number, chemistry and mechanical results agree EN 10204 3.1 / ASME CMTR
4. Cutting Master item becomes pieces Mark must be transferred to every cut piece Stencil / etch / tag
5. Fabrication Part is welded or machined Heat survives in the traveller and the part marking Traveler / router
6. Receiving Buyer checks the shipment PMI reading is recorded against the same heat PMI report + MTC

Notice that the physical mark and the document are separate things. The stamp on the bar can survive while the paperwork is lost, or the paperwork can be perfect while the mark has been ground off. Both are needed. Our EN 10204 3.1 certificate page shows the document side of the chain; this article is concerned with making sure the metal side still matches it.

If you are buying cut pieces, the marking question decides whether the rest of your traceability exists. Put these fields in the enquiry so every supplier answers the same question.

What to send us for an exact titanium quote

Copy these nine lines into your enquiry. A complete spec means a firm price on the first reply, not a second email asking for the grade.

Spec item Example from a real order
Grade Grade 2 (UNS R50400), commercially pure titanium
Standard ASTM B265 / ASME SB-265, current revision
Form & Size Plate, 6 mm × 1000 mm × 2000 mm, hot-rolled and annealed
Quantity 500 kg (12 sheets), one-off batch
Service medium & temperature Seawater, 30 °C, continuous immersion
MTC type EN 10204 3.1, heat-specific, with melt chemistry and tensile values
Inspection Third-party witness (SGS / BV) before dispatch; PMI on request
Target delivery Ex-works within 5 working days; FOB Shanghai on request
Drawing DXF of cut-to-size blanks, tolerance ±1.0 mm, edges deburred

Ready? Copy the nine lines above into the Requirement Details box on our Request a Quotation page and we will come back with a firm price and a dispatch date within 24 hours.

5. Where the Chain Breaks: Cutting and Cut-to-Size

Cutting is the highest-risk step in the whole chain. A certified master plate arrives with a legible heat stamp. It is cut into twenty rectangles. Unless the mark is transferred to each piece, nineteen rectangles have no identity, and no amount of later testing can tell you which certificate they belong to. Small pieces, fittings, machined parts and offcuts are the usual casualties.

The fix is a marking-transfer protocol: before cutting, record the heat number, transfer it by stencil, etch or tag to every piece, and keep a piece list that maps each cut item to the master heat. Some suppliers add PMI verification after cutting as a second gate. If your order is cut-to-size and the supplier cannot describe this step, assume traceability stops at the saw. Our small-batch cut-to-size page and fitting stock page show how we handle the small-piece case.

6. MTR Versus PMI: Paperwork Compliance and Physical Evidence

These two documents answer different questions and buyers routinely treat them as interchangeable. A mill test report says what the producer measured and recorded at the melt. A PMI report says what an instrument measured on a piece of metal at a point in time. Neither makes the other redundant.

A lookup table can tell you which certificate format belongs to which market: our certifications page lists the standards we work to, and the fitting MTC page shows a heat-numbered certificate at piece level. The important operational rule is simpler: every PMI reading must carry the heat number and the certificate reference. A PMI report without them is a chemistry result with no chain, and an inspector is entitled to reject it.

7. What a Handheld XRF Gun Actually Reads

Handheld X-ray fluorescence excites atoms in a thin surface layer and reads the characteristic energy each element emits. It is fast, non-destructive and good at the heavier alloying elements that separate most titanium grades. It is much weaker on light elements, and the grade name on the screen is a library inference, not a conformance decision.

Grade / case What the gun sees What it establishes What it does not establish
Grade 2 / CP Ti matrix, low Fe; no Al or V peak Confirms no alloy addition Does not confirm O / Fe within grade limits
Grade 5 (Ti-6Al-4V) V around 4%, Al around 6% Vanadium is the reliable separator Al accuracy is instrument- and surface-dependent
Grade 9 (Ti-3Al-2.5V) Lower Al and V than Gr5 OES preferred for the smaller peaks Grade library match can mislabel
Grade 7 Palladium present Pd is a clear marker Confirm Pd level against the specification
Grade 12 Nickel and molybdenum present Ni and Mo markers are readable Lab chemistry for exact limits
Grade 23 (ELI) Same Al/V as Grade 5 XRF cannot separate ELI from standard Lab O, N, H analysis required
Non-titanium substitution Wrong base elements Obvious mismatch is caught fast Read element values, not the grade label

Read the element values, not the label. Published PMI guidance notes that a gun may call one overlapping alloy by another grade name when the distinguishing element is outside its capability. The numbers are the evidence; the name is a conclusion drawn from a library that may be thin. For the chemical basis of the grades themselves, see our Grade 5 bar page and Grade 2 plate page.

8. What XRF Cannot See — And Why Buyers Over-Trust It

Three limits matter in titanium procurement. First, handheld XRF cannot measure carbon, nitrogen, hydrogen or oxygen reliably. That is why it cannot separate Grade 5 from Grade 23 ELI, or Grade 1 from Grade 4 where oxygen and iron limits define the grade. Second, it does not see heat treatment condition: annealed and STA material can read identically. Third, it analyses only a thin surface layer, so scale, paint, plating and heavy oxidation distort the result.

Question Handheld XRF Spark OES Laboratory method
Alloying elements (V, Mo, Ni, Pd, Fe) Yes, on clean bare metal Yes, broader light-element coverage Yes
Carbon, nitrogen, hydrogen, oxygen No — too light for handheld XRF Partly, method-dependent Yes — combustion / inert-gas fusion
Heat treatment condition (annealed vs STA) No No Mechanical test + metallography
Yield and tensile strength No No Tensile test to the named standard
Internal soundness No — surface layer only No Ultrasonic inspection
Which certificate covers this piece No — only the heat number answers this No Document review against heat number

One consequence deserves emphasis. A part can pass PMI and still fail in service because the heat treatment was wrong. That is the same territory our annealed versus STA guide and fatigue guide cover: condition and surface state set properties that a chemistry reading never touches. PMI is a gate, not a qualification.

If you need a supplier to state the marking and PMI scope in writing before you place the order, send the grade, form, certificate type and cut pattern through our request a quotation page. A named engineer will confirm what we can document from stock within 24 hours.

9. OES, LIBS and the Laboratory: Choosing the Referee Method

Spark optical emission spectrometry measures light elements that XRF misses and is the usual next step for questions such as aluminium and vanadium levels in Ti-3Al-2.5V. It leaves a small burn mark, so the location must be agreed before it touches a finished face. Handheld LIBS can measure some light elements too, but many specifications still name OES, so get acceptance in writing first.

For interstitial elements and for any dispute, the laboratory is the referee. Combustion and inert-gas fusion methods quantify oxygen, nitrogen and hydrogen with a reported uncertainty, and arbitration should rest on those results with calibration records rather than a field screening reading. Near-boundary XRF results deserve the same treatment: a longer count, a prepared surface, several locations, and then the named referee method if the result still matters.

10. The Other Mix-Up Path: Weld Consumables

A common verification programme checks the plate, the pipe and the fittings, then forgets the filler wire. A correctly verified base material joined with the wrong consumable fails at the weld just as readily as if the base material had been wrong. API RP 578 therefore includes weld consumable verification in a complete material verification programme.

In practice this means keeping filler wire in marked, segregated containers, recording the lot against the weld procedure, and verifying it before use where the specification calls for it. Our welding wire page lists the consumables we supply, and the flange with RT report page shows how inspection evidence is documented at the equipment level. Traceability that stops at the parent metal is only half a programme.

11. Industry by Industry: What “Enough Traceability” Means

The right level of evidence depends on what the part will do. A chemical vessel and an implant do not need the same package, and paying for the strictest option on a general utility part is as much a mistake as accepting the loosest one on a certified component.

Sector Typical requirement What to specify
Aerospace Individual-piece traceability, AMS material specs, AS9100 quality system, ultrasonic inspection Name the AMS spec and require per-piece marking; do not accept a generic "titanium"
Medical implant ELI chemistry under ASTM F136 / ISO 5832-3, biocompatibility and device records Lab interstitial analysis, not XRF alone, for Grade 23
Pressure vessel (ASME VIII) ASME-certified mill, code CMTR, authorised inspector acceptance Confirm the ASME certification and heat marking before fabrication
General chemical / industrial EN 10204 3.1 MTC with heat number is usually sufficient Agree marking transfer for cut pieces in the order

The aerospace row is where buyers most often underestimate the paperwork. Individual-piece traceability, an AMS material specification, a quality system and ultrasonic inspection are separate requirements that all have to be named. Our aerospace fastener bar page and fitting grade guide show how much of the detail sits in the order rather than in the grade name. When in doubt, ask the customer’s quality department for the material clause instead of guessing.

12. What To Do When the Goods Arrive

Eight checks turn a shipment from a pile of metal into a documented lot. They apply to stock material; certified aerospace or pressure-vessel work adds the inspection and sign-off requirements of the governing specification.

Step Why it matters Action
1. Match the certificate Heat number on the MTC must match the mark on the metal Reject if absent or inconsistent
2. Check the physical mark Stamp / etch / tag still present after cutting and packing Ask for the transfer record
3. Prepare the surface XRF reads only a thin surface layer Grind a small window to bright metal
4. Read elements, not the label Grade name on screen is a library match Compare values to specification limits
5. Check near-boundary results Every reading carries uncertainty Longer count, multiple spots, then escalate
6. Test weld consumables too Correct plate with wrong filler still fails API RP 578 covers consumable verification
7. Send ELI / interstitial questions to a lab Handheld XRF cannot see O, N, H, C Require witnessed lab analysis
8. Quarantine a fail A fail is a result, not a bad reading Isolate, re-check, follow the escalation procedure

Step 5 is where judgement matters most. Every instrument reading has uncertainty, and a result close to a specification limit is a prompt for more work, not a verdict. Step 8 is the discipline buyers skip: a failed reading is a result to be investigated, not a number to re-shoot until it passes. Related receiving checks for specific forms are covered on our plate receiving page, tube inspection page, bar receiving page, flange marking page, fastener lot page and wire inspection page.

13. Limitations: Where This Guide Stops

Traceability is a contractual and inspection subject, and there are cases where this guide cannot decide anything for you.

Situation Why this guide is not enough What to do instead
Safety-critical or code-certified part A supplier guide cannot replace the approved specification and inspector Use the governing code and an authorised inspector
Grade 5 versus Grade 23 ELI Same major elements; difference is interstitial chemistry Lab inert-gas fusion / combustion analysis
Heat treatment or strength question Chemistry does not establish condition or properties Mechanical test and heat-treatment record
Close-to-limit XRF reading Reported uncertainty is not a conformity decision Longer count, prepared surface, referee method
Old stock with no surviving mark The chain cannot be reconstructed by testing alone Treat as untraceable; do not certify by PMI
Zirconium or nickel alloy parts Different marker elements and acceptance limits Use the right material programme

The fifth row is the hardest one. Old stock with no surviving mark cannot be made traceable by testing it; a chemistry result says what the metal is, not which melt it came from or which certificate covers it. The honest answer is to treat it as untraceable and not write a certificate it cannot support. Our equipment arrival acceptance guide covers the wider acceptance sequence once material identity has been established.

14. A Twelve-Line Traceability RFQ Checklist

Send these fields together and a supplier can answer with a real documentation plan. Line 5 is the one that protects cut-to-size orders; line 12 is the one that decides what happens when something does not match.

# Field Example entry
1 Exact grade and product form Gr2 plate / Gr5 bar / Gr7 fitting
2 Governing standard and edition ASTM B265 / ASME SB348 / AMS 4928
3 Certificate type required EN 10204 3.1, 3.2, ASME CMTR
4 Marking method Stamp / etch / tag; location on the part
5 Cut-to-size marking transfer Every piece marked, with a transfer record
6 PMI scope and method XRF or OES; per heat / per batch / per piece
7 Acceptance limits and source Your specification, not the generic grade range
8 Interstitial analysis if ELI / medical Lab O, N, H with reported method
9 Weld consumable verification Filler grade and PMI requirement
10 Inspection beyond chemistry UT, PT, dimensional report
11 Document package at shipment MTC, PMI report, heat list, packing list
12 Rejection and escalation route Quarantine, re-test, who authorises release

Line 7 deserves a note: acceptance limits should come from your own specification, not from the generic grade range in a handbook. The instrument enforces whatever limits it is told to enforce, so a loose default setting can produce a “pass” that your design does not accept. Writing the limits into the order is what turns PMI from a demo into a contractual check.

15. Choose Standard Stock / Choose Verified Lot / Choose Full Chain

Choose standard stock with an EN 10204 3.1 MTC if the part is general chemical or industrial service, the full mill form is supplied, and the heat number on the certificate matches a visible mark. This covers most plate, tube and bar orders.

Choose a verified lot with defined PMI and marking transfer if you cut to size, buy small fittings, or receive material through several handlers. Require per-piece identity and a stated acceptance method; this is where most mix-ups become possible.

Choose full chain with individual-piece records if the part is aerospace, medical implant or code-certified pressure equipment. Name the AMS, ASTM F or ASME requirement explicitly, and include laboratory interstitial analysis and weld consumable verification where the specification calls for them.

16. Why Source This From Us

We are a stockholder plus light fabricator in Baoji, the centre of China’s Titanium Valley. We will not answer “full traceability” without saying what that means for your order:

  • Heat-numbered stock. About 800 t of titanium, nickel and zirconium across plate, tube, bar, wire, fittings, flanges and fasteners, with the certificate tied to a named heat.
  • Cut pieces keep their identity. Marking transfer on cut-to-size orders, with a piece list back to the master heat — the step most often skipped.
  • PMI on request, with limits agreed. XRF or OES as the question requires, reported against the heat number and your stated acceptance limits, not a generic grade label.
  • Honest scope. We will say when a question needs a laboratory, a tensile test or ultrasonic inspection rather than presenting a gun reading as proof of everything.
  • Fast where it counts. Technical answers and pricing within 24 hours, stock sizes dispatched the same day, export packing and documents handled in house.

Start with Grade 2 plate, Grade 12 plate, Grade 5 bar, fittings or nickel alloy stock; each page lists the forms, sizes and certification that matter for that product.

Get a firm titanium quote within 24 hours

Same-day dispatch from ~800 t of Baoji stock  ·  cut-to-size and waterjet blanks  ·  free drawing review by our engineering team  ·  EN 10204 3.1 MTC with every lot.

Request my quote →

No obligation. A named engineer replies, not an auto-responder.

EN 10204 3.1 MTC on every lot  ·  ISO 9001 quality system  ·  ASTM / ASME / GB standard literacy  ·  Third-party inspection (SGS / BV) on request  ·  Mill heat & lot traceability  ·  Export packing & full documentation

17. FAQ: Titanium Traceability and PMI

Can you tell Grade 2 from Grade 5 titanium by looking at it?

No. Commercially pure titanium and Ti-6Al-4V can have the same mill, pickled or polished finish, and their densities are close at about 4.51 and 4.43 grams per cubic centimetre, a difference under two percent. Neither is magnetic, and file or spark tests are subjective and unreliable. The reliable route is a chemistry measurement, normally handheld XRF or OES on metal cleaned to a bright surface, read against the specification limits.

What is a heat number and why does it matter?

A heat number is the mill identifier for one melt. Chemistry and mechanical test results are recorded against it, and the mill certificate names it. Without that number a measurement on a piece of metal is an isolated reading with no certificate behind it, and a receiving inspector is entitled to reject it. The heat number is the link between the physical material and the paperwork.

Can handheld XRF tell Grade 5 from Grade 23 ELI?

No. Both are Ti-6Al-4V with essentially the same aluminium and vanadium content. Grade 23 is defined by extra-low interstitial limits for oxygen, nitrogen and hydrogen, and handheld XRF cannot measure those light elements. Separating them requires laboratory combustion or inert-gas fusion analysis with a reported method. Treat any supplier claim that a gun can certify ELI as a specification gap.

Does a PMI test replace a mill test report?

No. The mill report is the record of what the mill tested at the melt; PMI is a check of the chemistry of the metal in front of you. One is document compliance, the other is physical evidence, and they are complementary. PMI also does not establish heat treatment condition, mechanical properties or internal soundness, so it cannot replace tensile testing, metallography or ultrasonic inspection where those are required.

How does traceability get lost after cutting to size?

A full-length plate or bar carries the mill marking, but once it is cut into twenty pieces, only the marked ones remain identifiable. Offcuts, small fittings and machined parts are the highest-risk items because the original mark is gone. The fix is a marking-transfer protocol: transfer the heat number and grade to every cut piece before it leaves the master item, and keep a record that ties each piece back to the certificate.

What standard governs a PMI programme?

API RP 578 is the widely cited recommended practice for material verification programmes on new and existing alloy piping, and it covers weld consumables as well as base metal. ASTM E1476 is a guide for metals identification, grade verification and sorting, and it distinguishes methods that measure composition directly from methods that respond indirectly to processing. For titanium the buyer should define the method, sampling rate, acceptance limits and reporting format in the purchase order.

What should I put on an RFQ to get real traceability?

State the exact grade and product form, the governing standard and edition, the certificate type, the marking method, and whether cut pieces must be individually re-marked. Define the PMI method and whether it is per heat, per batch or per piece, and set acceptance limits from your own specification. Add interstitial laboratory analysis for ELI or medical material, weld consumable verification, any UT or PT requirement, and the document package expected at shipment. Line 12 of the checklist in this guide, the rejection and escalation route, is the one most often left out.

Summary: Ask for the Chain, Not the Promise

A titanium certificate proves the paperwork; PMI proves the chemistry; only the heat number ties them together. Grade 2 and Grade 5 look the same and differ by under two percent in density, so sight, magnets and files cannot sort them. Handheld XRF separates grades by heavy elements such as vanadium, palladium, nickel and molybdenum, but cannot measure oxygen, nitrogen, hydrogen or carbon, cannot establish heat treatment condition, and reads only a thin surface layer. The chain most often breaks at cut-to-size, when an unmarked piece loses its certificate forever. Send the twelve-line checklist through our request a quotation page; a named engineer will confirm in writing what we can document from stock within 24 hours.

Close-up of a laser-marked heat number and grade stamp on a <a href=https://www.sxqytd.com/product/titanium-plate.html target='_blank'>Titanium Plate</a> corner beside its mill test certificate

Titanium Weight Calculator — Quick Reference

All values use density 4.51 g/cm³ (commercially pure and most Ti alloys). For Gr5 / Ti-6Al-4V (4.43 g/cm³) multiply by 0.982. Figures are theoretical; actual weight varies with tolerance and surface condition.

1. Plate & Sheet — weight per square metre

Formula: kg/m² = thickness(mm) × 4.51

Thickness (mm) 0.5 0.8 1.0 1.5 2.0 3.0 4.0 5.0
kg/m² 2.26 3.61 4.51 6.77 9.02 13.53 18.04 22.55
Thickness (mm) 6.0 8.0 10.0 12.0 15.0 20.0 25.0 30.0
kg/m² 27.06 36.08 45.10 54.12 67.65 90.20 112.75 135.30

Per full sheet: kg = T(mm) × width(mm) × length(mm) × 4.51 ÷ 1,000,000.

2. Round Bar — weight per metre

Formula: kg/m = diameter²(mm) × 0.00354

Diameter (mm) 6 8 10 12 15 20 25 30
PREVIOUS:Titanium Maximum Service Temperature: Four Limits, Not One Numbe No next