| Specification | Topic: Zirconium in Sulfuric & Reducing Acid |
|---|---|
| Applicable Standard | Covers: H2SO4 window, H3PO4, acetic/formic, nitric limits, failure |
| Material Condition | Standard: ASTM B551, B523, B493, B366, ASME B16.5 |
| Inspection & Packaging | Service: H2SO4 concentrator, phosphoric, organic acid, pickling |
Product Description: Zirconium in sulfuric acid: concentration limits, reducing-acid envelope, Zr702/Zr705 vs C-276, failure zones, ASTM B551, RFQ checklist for acid service
Zirconium resists sulfuric acid only inside a window — roughly up to about 60% concentration at the boiling point (approx, and the window narrows as you push temperature or concentration), and most organic reducing acids such as acetic and formic at will. Outside that window it loses: concentrated sulfuric above ~70%, fuming / oleum, any oxidiser or fluoride, and strong nitric all defeat its zirconia film. The single number to remember is the ~60–70% wall: below it, zirconium is the economical fully-resistant choice; above it, or wherever an oxidiser appears, step to Hastelloy C-276 / C-22 or a lined system. We stock Zr702 and Zr705 across plate, tube, bar, fittings and flange in Baoji, cut and shipped with full mill certificate, so your sulfuric line runs inside the envelope for years. This guide covers the concentration / temperature window, Zr702 vs Zr705 in acid, equipment design, and exactly where zirconium must NOT be used — plus a 5-minute RFQ you can send today.
For the alloy picture across zirconium, titanium and nickel, see our materials matrix; if the service is reducing acid but milder, our titanium guide explains the cheaper option.
| Item | Zirconium / detail | Note |
|---|---|---|
| H2SO4, up to ~60% (approx), boiling | Zirconium: good | Its reducing-acid window |
| H2SO4, >~70% / fuming / oleum | Zirconium: fails | Use Hastelloy / lined |
| H3PO4, pure | Zirconium: good | Watch F⁻ / Cl⁻ impurities |
| Acetic / formic (organic, reducing) | Zirconium: excellent | Pharma-clean service |
| Nitric / strong oxidiser | Zirconium: no | Use titanium / Hastelloy |
| HF / fluoride | Zirconium: fails | Use Monel / nickel |
| Max temp in reducing acid | ~250°C (pressure-dependent) | Above ~540°C in air: no |
| Vs Hastelloy for H2SO4 | Zr cheaper in-window | C-276 broader envelope |
Sulfuric acid is the test that separates zirconium from vague “acid-proof” claims. Zirconium’s zirconia (ZrO₂) film is stable in REDUCING H2SO4 — the lower-concentration, oxygen-free regime — but as sulfuric becomes concentrated and oxidising (above ~70%, or fuming), the film breaks and attack begins. Organic reducing acids (acetic, formic) are easy wins, and pure phosphoric is fine until halide impurities appear. The rule that prevents failures: zirconium owns reducing acid below the concentration wall; above it, or wherever an oxidiser shows up, use Hastelloy or a lined system. We plan plate, tube and fittings from one grade so the loop stays in spec and the certificate stays in one envelope.
A process datasheet is easier to read than it looks once you extract four numbers. Start with concentration: up to about 60% sulfuric, boiling, is zirconium’s window; above ~70% or fuming, move to Hastelloy C-276 / C-22 or a lined system. Then temperature: the window narrows as temperature rises, so a 60% stream near its boiling point is a harder case than the same stream at 40°C. Then contaminants: fluoride or chloride ions can cause localised attack in phosphoric and organic acids, and any oxidiser (nitric, ferric, cupric) flips the medium from reducing to mixed — verify the worst-case, not the name on the drum. Finally pressure and wall: pick Zr705 over Zr702 when you want thinner wall or higher design stress. Three worked cases: (a) 50% H2SO4 at boiling, no oxidiser → Zr702, economical and fully resistant; (b) 80% hot sulfuric → Hastelloy C-22; (c) phosphoric with fluoride → confirm purity, otherwise Monel. Send us the four numbers and we return the grade.
| Grade | Composition | Use it for |
|---|---|---|
| Zr702 (R60702) | ~99.2% Zr+Hf, low O | Reducing H2SO4/H3PO4; max formability |
| Zr705 (R60705) | +2.5% Nb | Same acids, ~50% higher strength |
| 702 vs 705 in acid | Both fully resistant in-window | 705 for thinner wall / higher pressure |
| Cross-check | — | See zirconium vs Hastelloy for the metal choice |
For full grade chemistry see our zirconium grade notes.
A usable quote starts with a usable request. Put these on the enquiry so we return price and lead time instead of questions:
| Form | Typical size | Where it goes |
|---|---|---|
| Plate / sheet | Thk 0.5–50 mm | Concentrator shells, tube sheets, trays |
| Tube / pipe | OD 6–219 mm | Sulfuric bundles, transfer lines |
| Bar / rod | Dia 6–300 mm | Spargers, agitators, shafts |
| Fittings / flange | per B16.5 / B16.9 | Branch, turn, termination of the loop |
For sulfuric service, wall thickness and weld quality matter more than grade choice: design for the corrosion allowance inside the window, keep joints double-purged, and let us cut plate and tube to size so field welding is minimised. We kit the matching fittings and flange from one shipment so the whole loop stays in spec.
Each lot ships with an EN 10204 3.1 mill test certificate, heat-number traceable to the melt, to ASTM B551/B523/B658 as applicable. Condition is annealed per spec; PMI, UT or dye-penetrant can be added on the order. For fabrications we kit the matching fittings and flange from one shipment.
Zirconium is not “acid-proof for every acid.” It owns reducing acid below the concentration wall, but concentrated sulfuric above ~70%, fuming / oleum, any fluoride, and strong oxidisers (including nitric) defeat it. For those services step to Hastelloy C-276 / C-22 or a lined system; for hydrofluoric use Monel; for hot caustic use Ni200 / Ni201. Match the grade to the actual fluid.
Zirconium’s strength is its reducing-acid film; its limits sit exactly where that film breaks down. Read the failure map, then the joint notes.
| Medium / condition | What fails / the limit | Use instead / action |
|---|---|---|
| H2SO4 >~70% / fuming / oleum | Film breaks, rapid attack | Use Hastelloy C-276 / C-22 or lined steel |
| H2SO4 with oxidiser (HNO3, Fe³⁺) | Becomes oxidising; attack begins | Step to Hastelloy C-22 |
| H3PO4 with F⁻ / Cl⁻ impurities | Localised attack at impurities | Confirm purity; otherwise Hastelloy |
| Acetic / formic with halide salts | Halides can pit; otherwise fine | Keep halide salts low; verify |
| Nitric / strong oxidiser | Zirconium attacked (oxidising) | Use titanium Gr7 / Hastelloy |
| HF / fluoride in any acid | Rapid attack — absolute exclusion | Use Monel 400 / pure nickel |
| Air / oxidising gas above ~540°C | Oxidises and can burn | Zirconium is not a high-temp alloy |
The concentration wall is not a rumour — it is electrochemical. Below about 60% sulfuric stays reducing and zirconium’s film holds; push past ~70% or into fuming and the acid becomes oxidising, the film collapses and attack is rapid. Because real process acid carries impurities, always specify the worst-case concentration and the contaminant list (fluoride, chloride, oxidiser) rather than the name on the drum — that is what keeps the part inside the envelope.
Choose this if:
Choose that if:
Use zirconium for the reducing window and step up only when the window closes. Inside ~60% sulfuric, pure phosphoric, acetic or formic, zirconium is the economical fully-resistant choice; above the wall, or with any oxidiser or fluoride, move to Hastelloy C-276 / C-22 or a lined system. Matching the metal to the actual fluid beats buying the “best” metal every time.
Zirconium is held in Baoji across plate, tube, bar, wire, fittings and flange, cut to size and dispatched fast for standard sizes. Heavy-wall tube, large forged flange or special tempers lead a few weeks. Small MOQ applies — a single plate, one spool or a set of flanges is a normal order, and we kit the whole line from one shipment with one certificate pack.
| If the service is… | Then… |
|---|---|
| Tantalum | Excellent in most acids but 5–10× zirconium’s cost — use only where Zr envelope is exceeded. |
| Hastelloy C-276 / C-22 | Broader envelope for concentrated / oxidising sulfuric and mixed acid — use above Zr’s wall. |
| Titanium (Gr2 / Gr7) | Excellent in seawater / chloride; attacked by sulfuric — wrong for H2SO4, right for chloride. |
| Glass-lined steel | Temperature-limited and thermal-shock prone — zirconium is more robust inside its window. |
| Monel / nickel | For HF and hot caustic where zirconium fails. |
Where these metals actually go: Zirconium builds sulfuric-acid concentrators, HCl-recovery units, acetic and formic acid plants and heat-exchanger bundles, and we size the wall for the corrosion allowance inside its window so the part lasts the campaign. We also supply the full nickel family and Hastelloy so an acid line can be split by fluid: zirconium inside its window, Hastelloy or nickel where the medium exceeds it — and we kit the matching fittings and flange from one shipment so the loop stays in spec.
Zirconium in acid service welds readily but unforgivingly: any oxygen or contamination during welding produces a hard, brittle, badly corroding joint. Use matching filler and a qualified WPS with argon backing gas on BOTH the inside and outside of tube and pipe, and keep the joint and wire clean. After welding, straw tint is acceptable; blue or grey means reject and re-pickle. We supply the matching wire and forming notes — a contaminated zirconium weld is the most common field failure, so do not skip the purge. See our welding guide for the full procedure.
Every lot ships with an EN 10204 3.1 MTC: grade and UNS, heat number, chemistry (including hafnium, which affects nuclear grade), tensile result, and the ASTM specification. Keep the heat number — it is your traceability link from the finished part back to the melt, and what lets an auditor confirm grade years later.
We hold zirconium together with titanium and nickel / Hastelloy in Baoji, close to China’s Titanium Valley supply base, which means we can cut, forge and kit an acid loop from one shipment instead of chasing several mills. That shortens lead time from mill-weeks to days and keeps one grade logic, one certificate pack, and one point of contact. Our guide explains the stock-holder model for overseas buyers.
Specifying the right grade is half the job; getting it delivered certified and on time is the other half. From Baoji, at the edge of China’s Titanium Valley, we hold zirconium with titanium and nickel / Hastelloy and turn a fluid spec into a shipped, certified line:
Start with the sulfuric envelope guide, then send the RFQ below — we confirm stock and pricing within 24 hours.
Copy this into your enquiry and fill the blanks — it returns a quote, not a guessing game:
Email it to [email protected], or use our inquiry form. We confirm stock and pricing within 24 hours; stock sizes can dispatch the same day, and fabricated items ship on a firm lead time we quote up front. Either way the whole line is kitted from one Baoji shipment so grade and certificate stay consistent end to end.
Zirconium resists sulfuric acid inside a window — roughly up to about 60% concentration at the boiling point (approx, and the window narrows as you raise temperature or concentration). Above about 70%, and in fuming or oleum sulfuric, the film breaks and zirconium is attacked; for those use Hastelloy C-276 / C-22 or a lined system.
Pure phosphoric acid (H3PO4) is fine for zirconium, but watch impurities: fluoride and chloride ions can cause localised attack. If the phosphoric stream carries halides or oxidisers, verify per case or step to Hastelloy.
Zirconium is excellent in acetic and formic acid and other organic reducing acids, and is a common choice for pharma-clean and food-grade duty. Keep halide salts low, as they can pit.
Dilute sulfuric is a reducing acid where zirconium’s zirconia film is stable; concentrated and fuming sulfuric becomes oxidising, which breaks that film and starts attack. The switch happens around the 60–70% range, so confirm your actual concentration.
Inside zirconium’s window (up to ~60%, reducing) zirconium is usually the cheaper fully-resistant choice. Above that, or wherever an oxidiser is present, Hastelloy C-276 / C-22 earns its premium with a broader envelope.
GTAW with matching filler and argon backing gas on both sides of the joint; any contamination makes the weld brittle and corrosive. We supply the matching wire and a qualified WPS note — see our welding guide.
Yes. Baoji stock to global ports with VCI protection, crating and full EN 10204 3.1 MTC and shipping documents.
If you take one thing from this guide, take this: specify the metal for the fluid, not just the word “corrosion-resistant,” and treat every joint as a system. Zirconium in Sulfuric & Reducing-Acid Service covers the sulfuric-acid and reducing-acid envelope of zirconium, and it should never be specified where the failure map says no. The fastest next step is concrete: copy the RFQ template above, or open our inquiry form, and send your medium, concentration, temperature and drawing. We confirm stock and pricing within 24 hours — stock sizes dispatch the same day.
Tell us your requirement — grade, size and quantity. We reply within 24 hours.
Prefer chat? WhatsApp +86 188 2967 9311 or email [email protected].
Contact Person: Wang Xiaoning
Tel: +86-917-355-7966
Email: [email protected]
WhatsApp: +86 188 2967 9311
Company: Shaanxi Qianyi Tuoda Technology Co., Ltd
Address: Floor 4, Building 4, No. 188 Gaoxin Avenue, High-tech Zone, Baoji City, Shaanxi Province, China